Home / Materials / HP HR PA 12 Glass Beads
HP HR PA 12 Glass Beads
PA12PowderMJFHP
Quick answer
HP 3D High Reusability PA 12 Glass Beads is HP's glass-bead-filled MJF powder: 40% glass beads in PA12, with 30 MPa tensile strength, 2800 MPa tensile modulus (XY) and 6.5% elongation at break, per HP's technical data sheet (4AA7-0716ENE). HP specifies a refresh ratio of 30% for stable performance — the stiffness grade of the MJF nylon line.
This is the MJF counterpart of the glass-filled SLS grades: where unfilled HP PA 12 balances strength and ductility (54 MPa, 18% elongation in the current sheet), the glass-bead grade trades ductility for stiffness and dimensional stability — modulus rises to 2800 MPa (XY) while elongation falls to 6.5%. HP positions it for enclosures and housings, fixtures and tooling.
The filler is spherical glass beads, not fibres — the same distinction EOS draws for PA 3200 GF — which is why the XY and Z figures stay close (modulus 2800 vs 2900 MPa, elongation 6.5% in both directions). The heat numbers are the other headline: HDT of 121 °C at 1.82 MPa and 173 °C at 0.45 MPa (Z, ASTM D648), well above unfilled MJF PA12 behaviour.
Properties (manufacturer datasheet)
| Property | Value | Orientation / condition | Test standard / note |
|---|---|---|---|
| Tensile strength | 30 MPa | XY | ASTM D638 |
| 30 MPa | Z | ASTM D638 | |
| Tensile modulus | 2800 MPa | XY | ASTM D638 |
| 2900 MPa | Z | ASTM D638 | |
| Elongation at break | 6.5 % | XY | ASTM D638 |
| 6.5 % | Z | ASTM D638 | |
| Heat deflection temperature | 121 °C | Z | ASTM D648 · @ 1.82 MPa |
| 173 °C | Z | ASTM D648 · @ 0.45 MPa | |
| Density | 1.3 g/cm³ | ASTM D792 · Printed part | |
| Melting temperature | 186 °C | ASTM D3418 | |
| Glass bead content | 40 % | Glass beads, per HP data sheet | |
| Izod impact strength (notched) | 2.7 kJ/m² | XYZ | ASTM D256 |
| Further values, as published (ranges & text) | |||
| Glass bead content | 40% | Glass beads, per HP data sheet | |
| Izod impact strength (notched) | 2.7 kJ/m² | ASTM D256, XYZ | |
Values are reproduced from the manufacturer source(s) listed below, exactly as published. Properties the manufacturer does not publish are omitted rather than estimated — see the sourcing policy.
Processing notes
- MJF powder for HP Jet Fusion systems; the data sheet lists compatibility with the Jet Fusion 4210/4200/3200 printing solutions.
- Refresh ratio for stable performance: 30% virgin powder, per the data sheet's recyclability table — equivalently, HP markets 70% surplus powder reusability for this grade.
- Average particle size 58 µm (ASTM D3451); powder melting point 186 °C (DSC, ASTM D3418).
Typical applications
- Enclosures and housings requiring stiffness and dimensional stability
- Fixtures and tooling
- Stiff functional parts where unfilled PA 12 flexes too much
Manufacturer, process & related entries
Manufacturer
HP Inc. is the US technology company founded in Palo Alto in 1939. Its Multi Jet Fusion (MJF) platform — the Jet Fusion printers and the High Reusability nylon powders — is one of the main production routes for nylon powder-bed parts, and the only MJF ecosystem.
Process
Inkjet arrays print fusing and detailing agents onto nylon powder and an infrared lamp fuses the printed areas, a whole layer in fixed passes.
Run the numbers for this grade
Two calculators read this database: the part cost estimator prices a part in this grade from its volume and datasheet density, and the refresh ratio calculator plans the virgin-powder blend for a build.
Frequently asked questions
What refresh ratio does HP specify for PA 12 Glass Beads?
30% virgin powder for stable performance, per the recyclability table of HP's data sheet (4AA7-0716ENE). HP phrases the same figure from the other side as 70% surplus powder reusability.
Glass beads or glass fibres?
Beads. HP specifies a 40% glass bead filling — spherical particles, which is why the XY and Z modulus and elongation figures are nearly identical. Fibre-filled grades behave more directionally.
PA 12 Glass Beads or unfilled HP PA 12?
Glass Beads when stiffness, dimensional stability and heat resistance dominate (2800 MPa modulus, HDT 121 °C at 1.82 MPa). Unfilled PA 12 when the part must flex or take impact — its elongation is 18% (XY) against 6.5% here, and its tensile strength is higher (54 MPa vs 30 MPa).
Sources
Last updated: November 2026